Latest News
BMC or SMC for Electrical Insulators: Three Checks Before You Choose

Date | 2026-11-16 14:31:55

— Same electrical ratings, a five-fold gap in tensile strength.

Inside low-voltage electrical equipment, BMC and SMC are often compared as if they were two grades of the same thing. They are not. One arrives as a bulk charge, the other as a sheet, and what they can be moulded into differs. Picking the wrong one can mean cutting a new mould.

The electrical numbers do not separate them: both sit at tracking index ≥600 V and electric strength ≥20 kV/mm. Tensile strength does — SMC-1 reaches ≥100 MPa, BMC 1615 reaches ≥20 MPa. So the question is not which material is better. It is which grade your part needs.

1. Start With the Part: Three Checks

Work through three checks in this order. Each one removes options.

Temperature. Above 130 °C, BMC 1616 and BMC 1615 drop out. What remains is all SMC grades, plus BMC 1625 and BMC 1620.

Load. Parts that carry assembly stress, absorb impact or span a large area go to SMC. Parts that mainly insulate, locate or separate are served well by BMC.

Shape. Cavities with many inserts, dense ribs or local thin walls favour BMC. Large parts with gentle curvature favour SMC.

Three checks usually settle it:




Part characteristicSMCBMC
Service temperature above 130 °CAll grades (≥155 °C)1625 and 1620 only
Carries assembly stress or impactSuitedLight-load parts only
Large area, gentle curvatureSuitedShort fibre, limited load capacity
Many inserts, dense ribs, local thin wallsWeak flow, short shots likelySuited
Insulation and location, little loadOver-specified, higher costAdequate

The sections below explain why each check sits where it does.

2. Why the Electrical Ratings Do Not Decide It

A common assumption says: if the requirement is high, use SMC. It does not hold. Both materials carry the same requirement values — tracking index, electric strength, arc resistance, insulation resistance — with no distinction between the two families.

The reason is simple. Both are unsaturated polyester systems reinforced with glass fibre. Electrical performance comes from the formulation, not from whether the fibre arrives as a sheet or as a bulk charge. "Which one insulates better" is therefore not a question worth asking. It is a threshold both clear.




PropertyRequirementNote
Tracking index (PTI)≥600 VSurface resistance to tracking under electric field and contamination
Electric strength≥20 kV/mmPower-frequency short-time breakdown
Arc resistance≥180 sHigh-voltage, low-current arc discharge
Insulation resistance, normal≥1.0×10¹³ Ω—
Insulation resistance, 24 h wet≥1.0×10¹² ΩOne order of magnitude retained after moisture uptake
Glow-wire flammability960 / 850 / 650 °CGrade dependent; 960 °C is the top band

Note: these figures are the minimums set in Wenzhou Jintong's internal standard Q/JTJ0001-2025 — the same document our outgoing inspection runs against. They are commitments rather than marketing numbers, and they apply to every grade in both families.

3. Mechanical Strength: Where the Gap Is

Tensile and impact strength are where the two families separate. SMC carries longer fibre with better orientation: SMC-1 reaches ≥100 MPa in tension, five times BMC 1615 at ≥20 MPa. Impact strength is ≥90 kJ/m² against ≥25 kJ/m², a factor of 3.6. This is not a marginal difference — it is a different class of part.

SMC grades:





PropertySMC-1SMC-2SMC-3
Tensile strength (MPa)≥100≥60≥55
Charpy impact, unnotched (kJ/m²)≥90≥60≥45
Flexural strength (MPa)≥170≥160≥140
Temperature index (°C)≥155≥155≥155

BMC grades:






PropertyBMC 1625BMC 1620BMC 1616BMC 1615
Tensile strength (MPa)≥35≥30≥25≥20
Charpy impact, unnotched (kJ/m²)≥40≥35≥30≥25
Flexural strength (MPa)≥140≥130≥110≥90
Temperature index (°C)≥155≥155≥130≥130

Note: values from the same internal standard. The tables are split so the trend inside each family stays readable — from SMC-1 to SMC-3, and from BMC 1625 to 1615, each is a single downward curve.

Read them in two steps. First, does the part carry load? Load-bearing parts, large panels and impact-resistant structures want the headroom SMC provides; parts that insulate, locate or separate are fine on BMC. Second, check temperature as a separate gate: all SMC grades and BMC 1625/1620 sit at ≥155 °C, while BMC 1616/1615 sit at ≥130 °C.

4. Shape Decides What Can Be Moulded

SMC is not the universal answer simply because it is stronger. It arrives as a sheet — good drape, weaker flow. That suits large parts with gentle curvature. BMC flows, so it fills cavities with dense ribs, metal inserts or local thin walls. The more complex the shape, the stronger the case for BMC. This check is not about performance; it is about whether the part can be made at all.



Process stepParameter
Mould temperature135–170 °C. Lower end for walls ≤3 mm, upper end for walls >5 mm; uniformity within ±5 °C
Low-pressure closing0.5–3.0 MPa at 10–20 mm/s
High-pressure dwell3.5–14.0 MPa, set by flow length and projected area
Cure time1.2–1.5 min per mm of maximum wall thickness
Charge weightTheoretical volume × flash allowance 1.05–1.15
Material storageSealed at 25 ± 5 °C, ≤60 % RH; shelf life applies after opening

Note: process window from Wenzhou Jintong's process specification Q/JTJ0002-2025, taken from production rather than calculated.

This check also carries the highest cost of being wrong. A cavity is designed around one material's flow behaviour; switching later usually means recalculating gate, venting and pressure gradient, which can amount to a significant mould change.

5. Cost, and One Trial Run

No universal price per kilogram settles this. Four variables drive part cost: grade (higher mechanical grades cost more to formulate), part weight and projected area (which set the press tonnage), mould complexity (inserts, slides, cavitation), and batch size together with post-processing.

The practical order is: settle the grade from temperature and load, confirm the shape can be moulded, then work out part cost from annual volume. Comparing unit price first tends to land on a grade that does not fit, and rework costs more than the saving.

Paper data narrows the range; it does not confirm it. Before locking a grade, run a small trial batch on the actual mould and measure dimensions, appearance and assembly fit. Wenzhou Jintong has worked in thermoset composites since 2001, with material, tooling and moulding in house, so a trial runs on the same chain that will produce the part.

6. Common Questions

Can SMC and BMC share one mould?

Usually not. A cavity is designed around one material's flow behaviour, and the two differ. Sharing a mould means designing for both windows before cutting steel, then proving it by trial.

Can parts of both materials be used on the same equipment?

Yes, decided part by part. Structural parts in SMC and insulating separators in BMC is a common combination. Both are unsaturated polyester systems, so thermal expansion and moisture behaviour are close, and one tolerance scheme can usually cover both. Final confirmation still comes from measuring the parts.

Which is more economical for small batches?

It depends on the part, not the batch size. At low volume the mould dominates cost, so the question becomes whether the mould can be got right first time. Complex parts with inserts stabilise faster in BMC; simple large parts need a simpler mould in SMC. Batch size changes amortisation, not material fit.

The part has inserts and carries load. Which way?

Size the mechanics first, then solve the moulding. If SMC's headroom is genuinely required, consider local reinforcement in the mould, repositioning inserts, or a higher-flow SMC grade. If the load is modest, BMC is the simpler route. This is the case most worth proving with a trial run.

For technical data sheets, grade recommendations, or a discussion about your specific requirements:
📧 wendy.qiu@smcbmc.com  📞 +86-13868305300